Oct 17, 2024 Tso lus

Dab tsi yog cov teeb meem thiab qhov tshwm sim uas yuav tshwm sim thaum siv Tin da dej hauv qab cib?

Cov xwm txheej tshwm sim los ntawm cov teeb meem zoo ntawm tin da dej hauv qabrefractory brickshauv kev tsim khoom tiag tiag yog cov hauv qab no.

 

tin bath bottom bricks


(1) Cov tin da dej hauv qab refractory cib npuas tuaj, thiab cov npuas ntab tuaj thiab cuam tshuam rau cov iav tsis khov, ua cov pits nyob rau sab saum toj ntawm iav (qhib npuas hauv qab phaj).
(2) Lub Na2O tso tawm los ntawm iav nkag mus rau hauv qab cib qauv, reacts tsim nepheline minerals, thiab yog nrog los ntawm ib tug ntim expansion ntawm txog 20%, thiab cov tshuaj tiv thaiv txheej curls thiab tev tawm thiab floats.
(3) Lub cev cib tawg kab rov tav, thiab sab sauv ib nrab ntab, feem ntau hu ua "7-inch effect" (1 nti=0.0254m).
(4) Hauv qab cib arches.
(5) Cov khoom sib khi yog delaminated thiab ntab, ua rau khawb rau ntawm qhov chaw qis ntawm iav.
(6) Cov bolts uas kho cov cib hauv qab yog corroded thiab melted los ntawm cov kua tin, thiab cov cib hauv qab ntab.
(7) Tin los ntawm hauv qab ntawm lub tank.
Qhov ua rau ntawm cov xwm txheej saum toj no tuaj yeem yog ib qho los yog sib xyaw ua ke ntawm cov hauv qab no.
(1) Cov dej cov ntsiab lus ntawm cov tin da dej hauv qab refractory bricks yog siab, thiab nws tsis tas drained thaum lub sij hawm cua sov thiab ci. Thaum qhov kub thiab txias hauv chav da dej hloov pauv thaum lub sijhawm tsim khoom, ntau cov npuas yuav tsim tawm. Cov npuas ntab tuaj thiab cuam tshuam thiab ua rau cov iav mos siv, ua kom muaj qhov tsis zoo ntawm cov npuas qhib hauv qab lub rooj tsavxwm. Tsis tas li ntawd, tom qab cov dej hauv qab ntawm da dej yog ci thiab sublimated, ntau dhau los ntawm qhov pores yog sab laug, thiab cov roj tin da dej tuaj yeem nkag tau yooj yim thiab ua npuas.
(2) Cov av nplaum zoo Cov tin da dej hauv qab cib absorbs Na2O los ntawm iav. Nyob rau ntawm qhov chaw sib cuag nrog cov kua tin, lub iav theem ntawm cov av nplaum cib reacts nrog Na2O los tsim nepheline minerals, nrog rau ntim expansion (20%). Thaum lub thermal expansion shear quab yuam tshaj lub zog ntawm lub cib, tus tshiab nepheline peels tawm thiab ntab li, ua rau iav tsis xws luag thiab shortening lub neej kev pab cuam ntawm lub tin da dej. Qhov teeb meem no feem ntau tshwm sim ib xyoos tom qab kev tsim khoom tau muab tso rau hauv kev ua haujlwm, uas yog ib qho ntawm cov teeb meem tseem ceeb uas plague lub neej kev pab cuam ntawm tin da dej hauv qab cib. Qhov laj thawj tseem ceeb yog qhov tin da dej hauv qab cib muaj huab cua permeability loj thiab muaj peev xwm tiv thaiv tsis zoo.
(3) Hauv xyoo 1970s, muaj ntau yam "7- ntiv tes tawg thiab ntab" kev sib tsoo ntawm cov pob zeb hauv qab txawv teb chaws. Nyob rau hauv kuv lub teb chaws, muaj arching xwm txheej ntawm qab cib nyob rau hauv ib co manufacturers. Qhov laj thawj tseem ceeb yog vim li cas tus nqi ntawm cov tin da dej hauv qab refractory bricks siv yog tsawg, feem ntau tsawg dua 0.5%, thiab cov pob qij txha ntawm cov cib kuj me me. Lub cib lub cev tau raug kev nyuaj siab heev, ua rau muaj kab rov tav tawg raws lub khob hliav qab ntawm qhov kho qhov ntsia hlau. Lub sab sauv ntawm lub cib lub cev ntab mus, thiab hauv qab cib nthuav dav vim cua sov los ua kom muaj kev ntxhov siab extrusion. Txhawm rau tso tawm qhov kev ntxhov siab, lub cib lub cev deformed thiab ua rau hauv qab cib arching kev sib tsoo.
(4) Muaj ob lub laj thawj tseem ceeb rau qhov tshwm sim ntawm cov khoom sib khi delamination thiab kev sib tsoo ntab. Ib qho yog tias cov khoom siv sealing tsis ua tau raws li qhov yuav tsum tau ua thiab tsis haum rau kev ua haujlwm ntawm cov khoom siv hauv qab cib. Lwm qhov yog kev tsim kho tsis raug. Txheej tamping ua rau cov khoom sib khi tsis sib xyaw ua ke zoo nrog lub hauv qab cib inverted cone qhov.
(5) Cov bolts uas kho cov cib hauv qab yog corroded thiab yaj los ntawm cov kua tin, thiab cov cib hauv qab ntab. Muaj ob lub laj thawj tseem ceeb:
Ib qho yog tias cov khoom siv ntawm kev kho bolts, graphite, sealing khoom, thiab lwm yam tsis ua raws li cov qauv tsim; lwm qhov yog kev tsim kho tsis raug. Cov laj thawj tseem ceeb yog: cov khoom sib khi ntawm lub khob hliav qab lub qhov ntawm lub hauv qab cib tsis kaw nruj nreem; lub qhov ncaj ntawm lub tin da dej hauv qab refractory bricks tsis kaw nruj nreem, ua rau cov kua tin nkag mus rau hauv lub qhov ncaj thaum qhov kub ntawm lub phaj hauv qab hloov pauv. Nyob rau hauv ib txwm muaj xwm txheej, vim huab cua txias hauv qab ntawm lub tank, qhov kub ntawm lub phaj hauv qab feem ntau qis dua 150 degree (qis dua qhov melting point ntawm tin). Txawm hais tias cov kua tin ntws los ntawm cov pob zeb cib mus rau hauv qab phaj, nws yuav khov thiab yuav tsis nkag mus rau hauv qhov ncaj. Txawm li cas los xij, nyob rau hauv cov xwm txheej txawv txav xws li hluav taws xob hluav taws xob thiab hluav taws xob hluav taws xob, lub phaj hauv qab tsis txias txaus, thiab cov kua tin nkag rau hauv lub qhov ncaj. Txij li thaum qhov kub ntawm lub bolt caj dab siab tshaj qhov melting point ntawm tin, lub tin yog nyob rau hauv ib tug molten lub xeev, uas tseem mus corrode lub bolt. Lub tin tank hauv qab phaj tsis tiaj tus, ua rau muaj qhov sib txawv loj ntawm lub phaj hauv qab thiab hauv qab cib. Graphite hmoov yooj yim nkag mus rau hauv qhov sib txawv thaum lub sij hawm tsim kho, ua rau nws nyuaj rau tamp cov graphite hmoov nyob rau hauv lub qhov ncaj, thiab cov nyhuv tsim yog ib qho nyuaj rau lav.

(6) Raws li qhov chaw tsim khoom ruaj khov, muaj ob qho laj thawj rau cov dej xau ntawm cov tin hauv qab ntawm lub tank. Ib qho yog cov vuam tsis zoo ntawm lub plhaub tooj liab nyob rau hauv qab ntawm lub tank; Lwm qhov yog tias sab sealing cov khoom tsis yog rammed nruj, ua rau cov kua tin tuaj yeem tiv tauj ncaj qha thiab corrode lub plhaub steel hauv qab ntawm lub tank.