Lub luag hauj lwm ntawm lub ladle nyob rau hauv lub steelmaking cog yog thauj cov hlau molten smelted nyob rau hauv lub converter mus rau lub nruam casting. Ntawm qhov nruam casting ladle turntable, 1500 degree high-temperature molten steel ntws tawm mus rau hauv lub tundish los ntawm lub nozzle thiab swb phaj nyob rau hauv qab ntawm lub ladle, thiab kev hloov ntawm lub billet yog ncua. Thaum kawg, nws ntws tawm ntawm lub tundish nozzle mus rau qhov nruam casting thiab straightening kom tiav cov billet forming. Rau lub nozzle uas kub-kub molten hlau ntws tawm ntawm lub ladle, nws yuav tsum tau muab tso rau hauv lub nozzle lub rooj cib. Thaum siv lub ladle, lub nozzle tuaj yeem hloov pauv hauv online 20-25 zaug. Lub nozzle lub rooj cib yuav tsum tau hloov thaum lub ladle yog kho rau me me. Hloov lub nozzle thaiv. Qhov zoo ntawm nozzle thaiv cib thiab qhov zoo ntawm kev tsim kho ncaj qha cuam tshuam seb lub ladle tuaj yeem ua haujlwm li cas. Cov teeb meem zoo ntawm ladle nozzle block bricks thaum lub sijhawm ua haujlwm feem ntau suav nrog cov khoom tsis ruaj khov, teeb meem hauv kev tswj cov txheej txheem knotting, tsis txaus ci, thiab qhov tsis xws luag hauv kev tsim kho thiab kev teeb tsa ntawm qhov chaw. Daim ntawv no txheeb tawm thiab daws cov teeb meem ntawm lub nozzle thaiv cib ntawm qhov chaw, thiab thaum kawg ua tiav cov txiaj ntsig zoo, ua kom lub cev ua haujlwm ntawm lub ladle.
1. On-site tej yam kev mob ntawm kev siv ladle
Ib lub tuam txhab steelmaking siv ib tug 150- tuj ladle nrog ob lub nozzles. Cov nozzles ncaj qha inlaid nyob rau hauv lub rooj zaum cib. Lub rooj zaum cib yog ntsia rau hauv qab ntawm lub hnab thaum tsim cov magnesia-carbon bricks nrog rau hauv qab ntawm lub hnab. Lub neej yog synchronized nrog hauv qab ntawm lub hnab, thiab lub neej kev pab cuam yog 70-80 furnaces Nyob nruab nrab ntawm lub sij hawm, tag nrho cov kev pab cuam lub neej nyob nruab nrab ntawm 130-150 furnaces. Lub ladle nozzle yog ntsia ua ntej lub ladle yog ci thiab mus online. Lub sealant yog siv rau sab nraud ntawm lub nozzle, thiab lub nozzle yog artificially inlaid mus rau hauv lub block ntawm lub zog siab, yog li ntawd lub block, cement thiab nozzle yog sib txuas nrog tag nrho, uas ua rau kom lub zog tag nrho. Thaum lub sij hawm siv lub thaiv, lub Uppermost ib feem ntawm lub block ncaj qha hu rau cov thawj feem ntawm cov hlau molten, lub nruam yaig thiab yaig thaum lub sij hawm lub outflow ntawm lub molten steel, thiab qhov ntev ntawm lub block yog luv luv. Qhov cuam tshuam ntawm qhov kub thiab txias molten steel, kev sib txhuam thiab kub sib txawv ntawm cov txheej txheem ntau lawm, kev sib txuas nrog lub rooj zaum cib yog kaw los ntawm cov kua nplaum sealing ntawm lawv. Txij thaum Lub Xya Hli mus txog Lub Cuaj Hli 2019, qhov tshwm sim ntawm cov kab nrib pleb hauv cov pob zeb ntawm lub nozzle thaiv tau tshwm sim ib zaug. Nws tau pom tias kev kho mob offline tau ua tiav nyob rau lub sijhawm, thiab nws tau pom tias cov hlau tho los ntawm cov cement channel ntawm lub nozzle thiab qhov thaiv tsis tau raws sijhawm, uas tau txwv nruj rau kev tsim khoom ntawm qhov chaw. Lub suab nrov nce tus nqi ntawm lub ladle, thiab kev tsim khoom yog nyob rau hauv qhov xwm txheej passive.
Lub hom phiaj ntawm kev sib tsoo ntawm cov hlau tsis sib haum ntawm cov channel thiab lub nozzle tshwm sim los ntawm kev tawg ntawm lub rooj cib, txheeb xyuas thiab taug qab ib qho los ntawm qhov zoo ntawm lub nozzle, muaj pes tsawg leeg, qhov zoo ntawm lub rooj cib, kev tsim kho, thiab lwm yam. tsis tu ncua, thiab qhov ua rau tuaj yeem txiav tawm; Pom cov kab nrib pleb, kev tsom xam feem ntau yog vim cov kab nrib pleb hauv qhov thaiv, qhov kev ncaj ncees tsis tiav, lub zog txo qis, thiab qhov sib txawv ntawm qhov thaiv thiab lub nozzle nce, cov hlau molten seeps rau hauv qhov sib txawv ntawm cov cement, thiab cov blocks, cement thiab lub nozzle yog txuas ua ke. Lub zog tag nrho raug rhuav tshem, thiab lub sealant tsis tuaj yeem tiv taus qhov kub thiab txias kub molten steel, thiab nws maj mam eroded, uas ua rau muaj qhov tshwm sim ntawm steel to thiab steel leakage xwm txheej.
2. Kev npaj thiab kev ntsuas rau steel to
Rau kev sib tsoo steel hlau los ntawm cov kab nrib pleb hauv cov block bricks, cov neeg ua haujlwm ntawm steelmaking cog thiab cov chaw tsim khoom ua ke nrog cov chaw tsim khoom los soj ntsuam cov laj thawj. Cov khoom ntawm tuam txhab uas muag nrog lub koob npe nrov yog sim tawm, qhov teeb meem yog raws li nram no:
1) Lub rooj zaum cib ntawm cov chaw tsim khoom A tau siv rau ntawm qhov chaw, thiab tom qab lub sijhawm (kwv yees li 60 zaug), micro-cracks tau pom, thiab sab saud ntawm lub rooj cib tau pom tseeb txoj kab uas hla;
2) Lub rooj zaum cib ntawm cov chaw tsim khoom B tau mus offline, thiab nws tau pom tias tseem muaj ntau qhov ntev ntawm micro-cracks, thiab cov kab nrib pleb tau muab faib ua 90 degrees nyob rau hauv nruab nrab ntawm lub rooj cib (cov neeg ua haujlwm los ntawm lub ladle kub kho platform ntsib lub lub rooj bricks raws li ib tug kab rov tav siv, thiab cov kab nrib pleb tsis nyob rau hauv lub rooj bricks. plaub fab).
3) Tus neeg ua haujlwm ladle tau txheeb xyuas cov khoom siv ntawm lub rooj zaum cib, xaiv cov khoom siv zoo rau cov qauv ua haujlwm ib kauj ruam, thiab kho cov qauv thiab cov khoom sib xyaw ntawm cov khoom sib xyaw thiab cov hmoov, thiab sau cov ntsiab lus hauv kev siv. Qhov tshwm sim ntawm cov kab nrib pleb maj mam tshwm sim. txo;
Cov kev ntsuas coj los rau kev teeb tsa thiab kev ua haujlwm ntawm lub rooj zaum thaiv yog raws li hauv qab no:
Lub rooj zaum cib yog tsim ua ke nrog rau hauv qab ntawm lub pob thaum lub sij hawm installation. Ua ntej lub rooj zaum cib raug teeb tsa thiab muab tso rau, cov qauv hlau nyob hauv qab ntawm lub rooj zaum cib yog ntxuav thiab ntim nrog impurities, thiab cov cheeb tsam ib puag ncig yog vibrated thiab ntim nrog castables, thiab ci tom qab kev tsim kho tiav, mus online, cov schematic tshwj xeeb. Daim duab qhia tau pom hauv daim duab hauv qab no:
1) Cov dej-cement piv ntawm cov castable nyob ib ncig ntawm lub hauv paus cib yog tswj nruj heev, thiab cov dej noo tswj ntawm 6-8 feem pua.
2) Castable siv: Rau qhov sib txawv (30-100mm) ntawm lub rooj cib thiab hauv qab ntawm lub hnab, cov txheej txheem vibrating yuav tsum tau ua manually, thiab lub vibrating pas nrig yuav tsum tsis txhob siv los vibrating, thiaj li yuav zam tau kev vibration quab yuam ntau dhau thiab aggregate sinking.
3) Thaum hloov lub nozzle online, xyuas qhov tawg thiab yaig ntawm lub rooj zaum cib.
4) Tiv tauj teem sijhawm tsis tu ncua. Yog hais tias lub sij hawm rau lub ladle mus tawm ntawm lub rooj sib txoos kab ntau tshaj 30 feeb, theem nrab ci yuav tsum tau ua.
5) nruj me ntsis saib xyuas qhov kub thiab txias thaum lub sij hawm ladle ci, xaiv ib phau ntawv tshwj xeeb, feem ntau sau qhov kub ntawm txhua feem (hauv qab ntawm lub ladle, ladle phab ntsa, slag kab, ladle qhov ncauj), thiab xyuam xim rau cov pa tawm ntawm lub ladle nozzle thiab lub ladle phab ntsa thaum lub sij hawm ci.
6) Cov chaw tsim khoom, nrog rau lub tuam txhab cov neeg ua haujlwm hauv chaw ua haujlwm, teeb tsa kev npaj ua tiav rau kev tsim kho ntawm qhov chaw, thiab ua kev cob qhia tsis tu ncua.
3. Cov nyhuv tom qab hloov pauv
Los ntawm cov pej xeem kev sib raug zoo ntawm ob peb yam ntawm lub rooj zaum bricks rau ze li ntawm ob lub hlis, cov kab nrib pleb ntawm lub rooj zaum bricks maj mam txo thiab ploj, thiab cov kev pab cuam lub neej kuj nyob rau hauv lub controllable ntau yam. Cov kev taw qhia thiab cov nyhuv ntawm kev kho dua tshiab tau zoo dua, uas tiv thaiv kev tsim khoom raug mob thiab txuag cov nqi ntawm cov khoom siv refractory. .
4 Kev xaus
Lub steel-ua ladle yog ib qho cuab yeej tseem ceeb rau kev hloov cov hlau ua kua. Qhov zoo ntawm cov khoom siv hluav taws xob sab hauv thiab kev tsim kho zoo yog ncaj qha ntsig txog kev tsim khoom thiab kev nyab xeeb. Kev tswj hwm txhua hnub thiab kev xa tawm ntawm lub ladle xav tau cov neeg ua haujlwm ntawm txhua cov nroj tsuag steel raws li lawv tus kheej xav tau. Txhawm rau tshawb nrhiav thiab sau cov ntsiab lus ua haujlwm, cov kev paub saum toj no tuaj yeem tsim nyog siv thiab nce qib.